Nickel recovery from spent nickel catalyst.

2005 
A process for nickel recovery from a spent catalyst of definite composition has been developed using the hydro-metallurgical route. The processing steps includes direct sulphuric acid leaching followed by separation of iron as well as silica and other impurities. For a 152 μm particle size catalyst, extraction of about 98% nickel was achieved at 363 K in 2 h using a sulphuric acid concentration (v/v) of 8% and a pulp density of 10%. The dissolution of nickel followed diffusion-controlled leaching kinetics. Increase in temperature and sulphuric acid concentration resulted in increase in the nickel recovery. The activation energy for nickel dissolution was calculated to be 62.8 kJ mol-1. Finally, nickel was recovered as value-added products such as sulphide and oxalate with overall recovery of 90 and 88% of nickel, respectively.